Solution Coating material Coating technology Coating hardness HIT [GPa] Coefficient of friction (dry) vs. steel Max. service temp. [°C] Process temperature [°C]
MoN Sputter / Arc 15 – 35 depending on application - 800 -
Download
ta-C Arc > 40 0.1 - 0.2 450 -
Download
TiN Arc 30 +/- 3 ~ 0.6 600 < 350
Download
AlTiN Arc 30 +/- 3 ~ 0.6 900 < 350
Download
AlTiN Arc ≥ 20 0.4 - 0.5 - 250 - 300
Download
TiN:Ag Arc 25 - 29 ~ 0.5 - < 350
Download
a-C:H:W (WC/C) Sputter 8-12 / 12-15 0.1 - 0.2 300 < 250
Download
CrN Sputter 18 +/- 3 ~0.5 700 < 250
Download
a-C:H PACVD ~ 15 - 25 0.1 - 0.2 300 < 250
Download
CrN + a-C:H PACVD ~ 15 - 25 0.1 - 0.2 300 < 250
Download
TiAlN Arc 33 +/- 3 ~0.6 700 < 350
Download
TiCN S3p ≥ 35 ~ 0.6 - < 400
Download
ZrN (Zirconium Nitride) Arc 20 - 25 0.5 500 350
Download
TiN Arc 30 +/- 3 ~0.6 600 < 500
a-C:H:Me (WC/C) Sputter 10 - 15 0.1 - 0.2 300 < 250
Download
CrN + a-C:H:Me (WC/C) Sputter 8-12 / 12-15 0.1 - 0.2 300 < 250
Download
TiN + a-C:H PACVD ~25-35 0.1 - 0.2 350 250 - 350
Download
CrN Sputter 18 +/-3 ~0.5 700 < 250
Download
CrN Arc 25+/-3 ~0.5 700 500
Download
CrN Arc 18+/-3 ~0.5 700 -
a-C:H PACVD ~15-25 0.1 - 0.2 300 < 250
Download
a-C:H:W / a-C:H PVD / PACVD ~15-25 0.1 - 0.2 300 < 250
CrN / a-C:H PACVD ~15-25 0.1 - 0.2 300 < 250
Download
a-C:H:Si PACVD ~ 15-25 0.05 - 0.2 350 < 220
Download
TiAlN Arc 33 +/- 3 ~0.6 900 500
ta-C Filtered Arc 35 - 50 0.1 - 0.2 450 < 100
Download
TiAlN Arc 32 +/- 2 ~0.6 700 < 500
Download
a-C S3p 30 - 40 0.1 - 0.2 350 < 200
Download
CrN / a-C S3p 30 - 40 0.1 - 0.2 350 < 200
- - - - - -
Download
- - - - - -
Download
- - - - - -
Download
NiCrAlY (Ni, Ni/Co, Co) Arc 7 - 11 - 1200 400 - 500
- - - - - -
Download